Line Broadening
This sheet: https://xraytools.com/broadening?inst=0.08&k=0.90&lambda=1.541838
Page: https://xraytools.com/broadening
Powder peaks get wider when the crystallites get smaller — and also when the lattice spacings vary. Give the positions and widths you measured and the page takes the instrument out, applies Scherrer to each peak, and then separates size from strain the only way a single peak cannot: by how the broadening grows with angle.
- Before this
- A measured line has a width, which an ideal lattice would not give — that width is the whole subject. Peak fitting is where the numbers this page wants come from.
- You supply
- A wavelength, your instrument’s own width, and a list of peaks — each one a 2θ and a full width at half maximum in degrees. Three peaks are the minimum for a Williamson–Hall fit and they are worth more the more widely they are spread.
- Reading it
- Every answer comes in two versions, because taking the instrument’s width out of a measured width depends on the peak shape and a real peak is between the two limits: the answer is inside the bracket, not at either end. L is a coherently diffracting domain and not a particle size, K = 0.9 is a convention worth about ten per cent on its own, and the instrumental width has to be measured on a standard — the default here is a plausible diffractometer and is not yours.
Worked examples: size only, simulated at 15 nm · strain only, simulated at 0.30% · both at once, simulated at 25 nm and 0.15% · a varying instrument, read as a flat width · the same peaks, read with the resolution function
Earlier on the path: Powder Indexing Next on the path: Intensity Corrections On From a measured scan to sample information, step 3 of 4
Notation here: K — what each one means here
See also: Bragg Calculator · HKL Calculator · Peak Finding · Powder Indexing · Reduced Cell and Bravais Lattice
What each input changes
- The peaks
- Positions and widths. The spread of angles is what separates size from strain, so two peaks close together cannot do it however precisely they are measured.
- How the instrumental width is given
- One number, or a curve. A real diffractometer is at its sharpest at some middle angle and wider on both sides of it, which a single number cannot say — and subtracting a flat width from a pattern takes off too much at one end and too little at the other, which tilts the Williamson–Hall line rather than shifting it. The tilt is the microstrain, so that is the answer it damages first.
Teaching with this page
- Objective
- After this page a learner can separate crystallite size from microstrain, and say what neither of them measures.
- Start from
- this worked example
- Ask first
- The analysis returns a crystallite size of 24 nm for a powder whose grains are visibly micrometres across. Is something wrong?
- Watch for
- “Yes — the size must match what the particles measure”
- Then
- Intensity Corrections
Check yourself: The analysis returns a crystallite size of 24 nm for a powder whose grains are visibly micrometres across. Is something wrong?
No — a grain is not a crystallite Yes — the size must match what the particles measure
Line broadening measures the coherently diffracting domain: the region over which the lattice is unbroken. One particle can be a mosaic of many such domains, so a large particle made of small domains gives exactly this result, and it is not a contradiction. Nothing in a diffraction pattern can see a particle.
Input
Results
No peaks were given. Each line of the box is one peak: its 2θ and its full width at half maximum, both in degrees.
Where this comes from
- X-ray line broadening from filed aluminium and wolfram
G. K. Williamson and W. H. Hall, Acta Metall. 1953, 1, 22–31 · doi:10.1016/0001-6160(53)90006-6
The separation this page’s plot performs, in the paper that introduced it. The two contributions are told apart by their angular dependence alone — which is why several peaks are needed and why one is not enough, whatever its width. - A method of calculating the integral breadths of Debye-Scherrer lines
A. R. Stokes and A. J. C. Wilson, Proc. Camb. Phil. Soc. 1942, 38, 313–322 · doi:10.1017/S0305004100021988
Where L is defined as a mean column length, the thickness of the crystal perpendicular to the reflecting planes averaged over its volume, rather than a particle size — the distinction the table of traps on this page spends the most words on. - The diffraction of X rays by distorted crystal aggregates - I
A. R. Stokes and A. J. C. Wilson, Proc. Phys. Soc. 1944, 56, 174–181 · doi:10.1088/0959-5309/56/3/303
Where the strain term 4ε tan θ comes from: the breadth that a spread of lattice spacings adds, and why it grows with angle differently from the breadth of a small crystal. - Choice of collimators for a crystal spectrometer for neutron diffraction
G. Caglioti, A. Paoletti and F. P. Ricci, Nucl. Instrum. 1958, 3, 223–228 · doi:10.1016/0369-643X(58)90029-X
The resolution function this page offers instead of a single instrumental width: FWHM² = U tan² θ + V tan θ + W, which is what those three letters mean in every Rietveld program. Worth knowing what it was written about: neutron collimators, three decades before it became the standard empirical fit to a laboratory X-ray instrument’s measured widths.